酸洗钝化记录 Pickling and Passivating
指令号
Instruction No.
工件编号
工件名称
Parts Name
图号
Drawing No.
20210720001
/
/
20-040388- A
数量
Quantity
材质
Material
X2CrNiMo18-10
AISI 316L
6
Parts No.
酸洗钝化膏
开始时间
结束时间
温度
清洗压力
Pickling
Start Time
End time
Temp.
Washing pressure
passivation paste
OK
14:10
15:40
24℃
/
清洗程序说明 Washing process:
1. preparation: Before picking and passivation , we should check the surfaces.
准备工作: 在拣选和钝化之前,检查表面。
2. Degreasing: Laying on Paste---- Degreasing paste shall be spread on the weld and
surface vessel evenly. Keeping----- Degreasing paste should be holding 20~30 minutes on the
weld surface and 10~20 minutes on the part surface. Washing----- itswabbing shall be washed with
Pure Water.
脱脂: 涂膏——将脱脂膏均匀地涂抹在焊缝和表面容器上。保持—脱脂膏应在焊缝表面保持 20~30 分
钟,在产品表面保持 10~20 分钟。洗——要用纯水洗。
3. Procedure for pickling and passivation 酸洗钝化工序
3.1Laying on Paste----The acid pickling and passivation paste shall be spread on the weld surface
and vessel surface evenly.
涂抹——酸洗钝化膏应均匀地涂抹于设备表面和焊缝处。
3.2 Keeping----- The acid pickling and passivation paste should be holding 60~90 minutes on the
weld surface and 40~60 minutes on the surface.
保持——酸洗钝化膏应在焊缝上保持 60~90 分钟,表面保持 40~60 分钟。
3.3 Swabbing----- The surface shall be swabbed with the scouring pad。
表面用百洁布擦拭。
3.4 Rinse - rinse with plenty of pure water,
冲洗-用大量的纯净水冲洗
4. drying ------ the surface shall be swabbed up the water with cloth.
干燥——表面用水用抹布擦干。
实施人
Operator
日期
检查人
Checker
日期
刘洪
李娟
2021/7/20
2021/7/20
Date
Date